1. Verify pipe, fitting and controller compatibility
A 110 mm metric socket and a 4-inch IPS pipe belong to different size series. The IPS pipe has a 114.3 mm OD. Read the markings and measure the pipe before selecting the coupling. Check metric and IPS dimensions.
- Pipe and socket. Match material, actual OD and SDR or wall thickness to the fitting’s approved range. Use a diameter tape to check mean OD. Measure the widest and narrowest diameters at the same section to check ovality. Look for flat spots, deep gouges and a pipe end that tapers inward (toe-in). If the end is undersized, cut back to sound, full-size pipe and measure again.
- Fitting. Keep it sealed until assembly. Check the label and fusion barcode. When opened, inspect the bore, terminals and any visible windings for damage.
- Controller and power. Verify the output range, lead adapters, barcode support and temperature compensation required by the fitting. Match the generator and cables to the controller’s input requirements.
Scraping depth and finished OD
For projects using the POP001 procedure, these metric examples pair the required peel depth with the smallest permissible mean outside diameter after peeling (Issue 9, Tables 2 and 3). Check the limits for the fitting on your order before setting up the peeler.
| Nominal pipe OD | Minimum peel depth | Minimum mean OD after peeling |
|---|---|---|
| 90 mm | 0.20 mm | 89.4 mm |
| 160 mm | 0.20 mm | 159.4 mm |
| 250 mm | 0.30 mm | 249.3 mm |
| 400 mm | 0.30 mm | 399.2 mm |
2. Prepare the pipe in five steps
Cut square and deburr
Support the pipe. Use a PE pipe cutter or guided saw to make a 90° cut. Clear shavings and burrs from both edges so the pipe can seat fully.
Measure and mark the socket depth
Clean and dry a band wider than the socket and peeler travel. Measure the insertion depth for this fitting. Use a quick-drying, oil-free marker to crosshatch the area to be peeled. Let the ink dry before peeling.
Peel the full circumference
Use an approved mechanical peeler sized for the OD. Check that the tool produces a continuous ribbon of the specified thickness. Inspect the underside with a mirror. Crosshatching left inside the fusion zone shows where the blade missed. Check the blade, pipe shape and remaining OD before another pass.
Protect the prepared surfaces
Follow the cleaning procedure for the fitting. Where wiping is specified, use an approved fresh wipe, work in one direction within the peeled area and allow the cleaner to evaporate. Open the fitting at assembly and keep fingers off both jointing surfaces.
Re-round, insert and clamp
Measure ovality and re-round at the stage specified by the fitting maker, including before peeling when required. Re-mark the insertion depth so the line will remain visible at each socket edge. Seat both ends to their marks and support the aligned assembly without bending load.
3. Field troubleshooting before and during fusion
Use a controlled peeling tool. Sandpaper can leave oxide or grit behind. A file or utility knife can gouge the pipe.
| What the crew finds | Why it matters | What to do |
|---|---|---|
| Pipe stops short of the insertion mark | A size mismatch or oval pipe can prevent full contact. | Check actual OD and socket size. Measure ovality and use the specified re-rounding tool before assembly. |
| Peeler or clamp cannot turn in the trench | Limited clearance can leave part of the fusion zone unpeeled or unsupported. | Check tool dimensions and arrange safe working clearance or prepare the joint in a suitable position. |
| Mud, water or grease on the peeled pipe | Contamination can prevent PE surfaces from bonding. | Stop assembly. Shelter the joint and follow the fitting instructions for re-preparation. Check the remaining OD before any further peeling. |
| Controller reports a fault during heating | The required fusion cycle may be incomplete. | Record the fault, leave the joint restrained and follow the fitting maker’s interrupted-cycle procedure. Restart only if expressly permitted. |
4. Run the electrofusion cycle
Before switching on Check that water from the trench or pipe bore cannot reach the joint, the pipe is fully seated at both marks, and the clamps carry the load. Confirm the local temperature is within the fitting’s installation range.
- Connect the leads. Seat the correct adapters on clean terminals. Support cables so they do not pull on the joint. Keep the work area clear during heating.
- Verify the settings. Scan the fitting’s fusion barcode, distinct from its traceability code. For ISO 13950 barcode operation, confirm controller compatibility. Use manual entry only where permitted. Compare fitting identity, voltage and cycle data on screen with the label and instructions.
- Monitor and record. Start the cycle and watch for a completion message or fault. Record the result and end time. Keep the joint stationary as cooling begins.
5. Inspect the joint before releasing it
Check at the socket
Look for alignment, insertion marks at both edges and the indicator response described for this fitting. Cross-check the controller’s completion record.
Hold for review
Flag shifted marks, misalignment, escaping melt, exposed wire, an unexpected indicator position or a cycle fault. Isolate the joint for disposition under the project procedure.
Cooling and release. Record the earliest clamp-release time from the fitting instructions. Keep pipe supports and clamps in place for that interval and let the joint cool naturally. Handling, tapping and pressure testing may each have a later release time.
Traceability and pressure testing. Link the fitting ID, joint location, operator, ambient temperature, cycle log and cooling record. After the specified test wait and inspection sign-off, follow the project’s approved hydrostatic test plan for the assembled line.
Electrofusion preparation FAQ
Why use a rotary scraper instead of sandpaper or a utility knife?
A correctly sized rotary scraper removes a controlled layer around the full socket contact area. Sandpaper can leave oxidized patches or embed grit. A knife can gouge the pipe and leave an uneven fit.
How much of the pipe surface should I remove?
Use the peel depth specified for the fitting and pipe size. Measure the peeled ribbon with a micrometer, then check the prepared pipe with a diameter tape. Before taking another pass, confirm that the finished pipe will stay within the permitted OD range.
How can I tell whether a completed electrofusion joint is ready for testing?
Check the controller log, insertion marks, alignment and any visible melt leakage. An indicator shows a local response to heating and cannot prove joint strength. Record the cooling and test-release times and obtain the inspection sign-off required by the project.
Can Puhui quote matching fittings, preparation tools and a controller together?
Yes. Send the pipe OD and SDR, fitting types and quantities, site power and working clearance. Puhui can check scraper and clamp sizes, controller output and lead compatibility, then quote the matching package.